Applications
MWD/LWD tools, marine shafts, high-strength fasteners.
MATERIAL DATASHEET
High-strength condition of Nitronic 50; yield strength ~ 725–965 MPa or higher depending on bar size and cold work; non-magnetic.
| Designation | Reference |
|---|---|
| UNS | S20910 (HS condition) |
| Werkstoff Nr. | — |
| ASTM | A276/A479 (bar) |
| ASME | SA276/SA479 |
| EN/ISO | — |
| Others | XM-19 HS |
| Property | Value / condition |
|---|---|
| Yield strength Rp0.2 | ≥ 725–965 MPa (bar, HS condition) |
| Tensile strength Rm | ≥ 930–1100 MPa (typ.) |
| Elongation | ~ 15–25 % |
| Hardness | — |
Weight %
| Element | Cr | Ni | Mo | Mn | N | C | Si | P | S | Fe |
|---|---|---|---|---|---|---|---|---|---|---|
| Min | 20.5 | 11.5 | 1.5 | 4.0 | 0.20 | — | — | — | — | bal. |
| Max | 23.5 | 13.5 | 3.0 | 6.0 | 0.40 | 0.06 | 1.0 | 0.04 | 0.03 | bal. |
MWD/LWD tools, marine shafts, high-strength fasteners.
Supplied cold worked to strength; not hardenable by heat treat.
Good (strength affected).